含碳铬矿的造球及还原催化研究  被引量:4

BALLING AND REDUCING EXPERIMENTS OF CARBON-BEARING CHROMITE POWDER

在线阅读下载全文

作  者:徐荣军[1] 倪瑞明[1] 张圣弼[1] 马中庭[1] 

机构地区:[1]安阳钢铁公司,北京科技大学

出  处:《烧结球团》1995年第2期10-14,共5页Sintering and Pelletizing

摘  要:本文介绍了原料粒度、粘结剂用量、配碳量时铬铁矿球团生球性能的影响以及温度和还原时间对金属化率的影响,结果表明:1350℃还原15min,铬金属化率达90%以上;配碳量应比理论配碳量过量20%;用1:3的H2SO4对还原球团采用加热回流法溶样,解决了金属铬和金属铁的化学分析问题。Balling and reducing experiments of carbon-bearing chromite powder were carried out in laboratory. The effect of grain size of raw materials .amount of binder and carbon and other factors on the green pellet properties and the influence of reducing temperature and time on the metallization rate of carbon bearing chromite pellet were investigated.The results from laboratorial experiments have shown that the metallization rate of carbon-bearing chromite pellet of up to 90% and more can be reached under the r...

关 键 词:铬铁矿 含碳球团矿 直接还原 环转炉法 

分 类 号:TF703.52[冶金工程—钢铁冶金]

 

参考文献:

正在载入数据...

 

二级参考文献:

正在载入数据...

 

耦合文献:

正在载入数据...

 

引证文献:

正在载入数据...

 

二级引证文献:

正在载入数据...

 

同被引文献:

正在载入数据...

 

相关期刊文献:

正在载入数据...

相关的主题
相关的作者对象
相关的机构对象