摘  要:为满足用户提出的轴承钢棒线材轻拉交货的要求,通过对轴承钢棒线材的传统工艺和新工艺进行比较,认为关键是退火工艺的制定.摸索出适合不同状态的冷拉盘条软化到比较一致的强度水平时的退火工艺:在强对流罩式炉中加热到(780±5)℃,保温4~7 h,带冷却罩冷却到140℃或以下温度出炉.To satisfy customer’s requirements for bearing steel wire rod and bar to be delivered by light drawing process, Laying down annealing process is key after comparing traditional process and new process of bearing steel wire rod and bar. Annealing process that can intenerate cold drawing wire rod of different situation to identical strength lever is found.The process of bearing steel wire rod and bar is heated at (780±5)℃ in strong convection bell-type furnace, then keeping 4~7h, cooled down to or below 140℃ in cooling cover then comes out furnace.

关 键 词:轴承钢 棒线材 再结晶退火 研究 

分 类 号:TG356.3[金属学及工艺—金属压力加工]

 

参考文献:

正在载入数据...

 

二级参考文献:

正在载入数据...

 

耦合文献:

正在载入数据...

 

引证文献:

正在载入数据...

 

二级引证文献:

正在载入数据...

 

同被引文献:

正在载入数据...

 

相关期刊文献:

正在载入数据...

相关的主题
相关的作者对象
相关的机构对象