萃取法回收水厂污泥中铝的技术研究 Ⅱ.浆液萃取法  被引量:3

Alum Recovery from Waterworks Sludge by Solvent Extraction Using Bi-(2-ethylhexyl)phosphate Ⅱ.Slurry Extraction

在线阅读下载全文

作  者:徐美燕[1] 孙贤波[1] 赵庆祥[1] 

机构地区:[1]华东理工大学资源与环境工程学院,上海200237

出  处:《华东理工大学学报(自然科学版)》2007年第3期375-378,409,共5页Journal of East China University of Science and Technology

摘  要:以水厂污泥为原料,二-(2-乙基己基)磷酸为萃取剂,煤油为稀释剂,研究了浆液萃取铝回收技术。结果表明:含固率为5%的浆液直接采用P204-煤油萃取,在pH=5.0、cP204=0.5 mol/L、相比(VO∶VA)为1∶1的条件下,铝萃取率可达96.9%以上,萃取剂回收率达到98%以上。以5 mol/L硫酸作为反萃剂,相比5∶1的条件下经3级反萃,可回收97.6%的铝,且反萃液符合液态商品硫酸铝的质量标准,可作为混凝剂利用。Al present in a water treatment plant sludge (SiO2 54.6%, Al2O3 10.3%, organic matters 12.5%) may be recovered and recycled as liquid alum for coagulation treatment. A slurry (5% SS by weight) was first prepared by mixing the sludge in a bi-(2-ethylhexyl)-phosphate Cp204 and kerosene extractant mixture. Under the optimal conditions of pH=5.0, Cp204 =0.5 mol/L, and phase ratio Vo : VA= 1 : 1, 96. 9% of Al was extracted, by ion exchange of H^+ for Al^3+ , from the sludge. Al in the extraction liquor was then stripped by H2SO4 solution (5 mol/L) in 3-stage stripping at a phase ratio of 5 :1 ; 97.6% of Al was moved to the clear aqueous phase which was reusable in the waterworks. 98% of the P204/kerosene extractant was recovered by centrifugation of the emulsified phase at 7 000 r/min for 10 min.

关 键 词:水厂污泥 铝回收 浆液萃取 二-(2-乙基己基)磷酸 

分 类 号:X705[环境科学与工程—环境工程]

 

参考文献:

正在载入数据...

 

二级参考文献:

正在载入数据...

 

耦合文献:

正在载入数据...

 

引证文献:

正在载入数据...

 

二级引证文献:

正在载入数据...

 

同被引文献:

正在载入数据...

 

相关期刊文献:

正在载入数据...

相关的主题
相关的作者对象
相关的机构对象